AuSn 80/20 is the default choice for hermetic, flux-free die attach in laser diodes, LEDs and RF devices. It melts at 280 °C, wets gold and nickel metallisations without flux, and does not outgas the way organic adhesives do. The complications are all in the preform: thickness, tolerance, oxide and how it is packed.
Why AuSn 80/20
| Composition | Au 80 / Sn 20 wt% — the eutectic point |
|---|---|
| Melting point | 280 °C eutectic (no pasty range — it melts and freezes at one temperature) |
| Why flux-free matters | No flux residue inside a hermetic package; no cleaning step after attach |
| Typical substrates | Au-plated or Ni/Au metallisation on the die and the package |
The parameters that actually cause defects
- Thickness tolerance — the preform sets the bond line. ±10% is normal; tighter on request. A thick preform can tilt a die, a thin one can starve the joint.
- Oxide on the surface — Sn oxidises. Vacuum packing with a short shelf life, or an oxide-free surface finish, is worth more than a higher purity grade.
- Burr and edge quality — stamped preforms carry burrs that hold gas; etched or laser-cut preforms do not.
- Area versus die size — a preform sized to the die footprint avoids overflow onto the bond pads.
Formats
| Preforms | Stamped, etched or laser cut to drawing; square, rectangular or round |
|---|---|
| Wire and ribbon | For hand or automated placement where a preform is impractical |
| Evaporation pellets | Same alloy for thin-film deposition of the solder layer |
Storage and handling
Store sealed, cool and dry. Open only just before use; do not handle with bare fingers. If the preform has been open to air for weeks, expect oxide and a slower, less even wet-out.
What we supply
- AuSn 80/20 evaporation pellets — 99.99%, for deposited solder layers
- AuSn preforms cut to drawing — quote against your die and package dimensions
- Solder materials and wires/foils — SnCu, SnAgCu and pure indium
Frequently asked
Can I reflow AuSn without flux?
Yes, provided both surfaces are gold or nickel-gold and the atmosphere is clean. Formic acid or a forming-gas reflow helps with oxide but is not always necessary.
What thickness should a preform be?
Usually 25–75 µm for power devices, thinner for small optoelectronic dies. The right value depends on the die size and the void tolerance of the joint — tell us both and we will suggest a range.
Do you supply AuSn with a specific oxygen content?
We can state it on the certificate; for die attach, surface oxide matters more than bulk oxygen.