Evaporation is simple in principle and fiddly in practice: the metal has to melt without spitting, wet the liner without reacting with it, and reach the substrate at a stable rate. These are the settings and habits that make the difference, whichever metal you run.

E-beam or thermal?

MethodE-beam — a focused electron beam heats the charge in a water-cooled hearth. Thermal — resistance-heated boat, basket or filament.
Use e-beam forHigh-melting metals (Ta, Mo, Re, W), oxides, and any material needing high rate and tight thickness control. The charge sits in its own liner, so contamination from the heater is not an issue.
Use thermal forAluminium, silver, gold, copper and other low-melting metals, especially in small or simple chambers where a boat is cheaper and faster to change.
Watch out forE-beam: beam striking the liner, poor thermal contact, splashing on first melt. Thermal: alloying with the boat, filament sag, spitting from an overheated spot.

Crucible liners and fill level

The liner protects the hearth and defines the usable charge volume. Graphite is the general-purpose choice; alumina and zirconia suit oxides and aluminium; tungsten or molybdenum liners are used where carbon contamination matters.

  • Fill 60–80% of the liner depth. Too little and the beam erodes the liner; too much and the melt can spill when it wets the walls.
  • Calculate by volume, not by eye. Pellets settle to roughly 55–65% of their bulk volume on melting, so a liner that looks full of pellets holds considerably less metal.
  • Use the crucible fill calculator to get the charge weight from liner dimensions, fill factor and density.

Pre-melt and degas

  1. Pump to base pressure and bake the chamber if the process allows.
  2. Raise the beam or boat power slowly until the charge just sinters — do not melt through immediately.
  3. Hold below melting for a few minutes to release adsorbed gas and moisture; pressure should fall back before you continue.
  4. Melt through, form a stable pool, then open the shutter. A steady pool gives a steady rate.

Rate and thickness

Quartz-crystal monitoring measures mass per area, so the tooling factor must be set for the geometry. Expect the first runs on a new material to need a calibration run: deposit a known thickness, measure it (profilometer or XRF), and correct the tooling factor.

To size the charge for a target thickness, use the film material calculator — it accounts for the material that misses the substrate.

Common defects and fixes

Spitting / particlesCharge contains gas or moisture, or the beam hits a fresh spot too hard. Pre-melt longer, ramp power more slowly, use denser pellets.
Poor adhesionSubstrate contamination or missing adhesion layer. Add a thin Ti or Cr layer, improve pre-cleaning and pump-down.
Rate driftPool shrinking, liner wetting, or beam position wandering. Top up the charge between runs and check the beam sweep.
Alloying with the boatAluminium and some low-melting metals react with tungsten. Use boron-nitride or alumina crucibles, or switch to e-beam.
Film contaminationLiner or boat outgassing. Use high-purity liners, bake out, and keep the charge covered between runs.

Documentation to ask for

For each lot: assay certificate with method and detection limits, trace-element table, and packing details. Request the SPEC sheet from the product page or by email.