E-Beam Evaporation Materials: Choosing Form, Purity and Liner

E-beam evaporation fails for reasons that are rarely about purity. Spitting, arcing, uneven melt and short liner life usually come down to the wrong form, the wrong liner, or a material that was never degassed. This page covers what to specify before you place an order.

Form: what each shape is for

Pellets Pressed or melted discs, typically 1–6 mm. Uniform melt, predictable fill level, good for production runs.
Granules Irregular pieces, 1–5 mm. Fill a liner densely, less bridging than large chunks, easy to top up.
Pieces / chunks Cut or broken material. Cheapest per kg, but initial melt is uneven and spitting is more likely.
Rods / slugs For specific source geometries; less common outside dedicated lines.

Purity: where the money actually goes

Each additional 9 raises cost steeply. The question is whether your process sees the difference:

  • 3N–4N is normally enough for decorative, wear and general metallisation.
  • 4N5–5N matters for optical films, where trace absorption shows up as loss.
  • 5N+ (and 6N for copper, aluminium, silicon) is for semiconductor and research work where a ppm-level impurity changes device behaviour.

Ask for the impurity table, not the headline number — “99.99%” without a stated basis (metals basis vs total, including or excluding oxygen) is not comparable between suppliers.

Liner choice by material

Aluminium Wets most liners and alloys with them. Use a BN or graphite liner and expect a single use.
Gold, silver, copper Graphite or BN; copper and silver can be run in a water-cooled copper hearth without a liner.
SiO2, TiO2, Ta2O5 Sublimating or low-thermal-conductivity oxides need a liner that insulates — graphite or BN — and slow initial heating.
Nickel, chromium, titanium Graphite works; these getter oxygen, so pre-melt and degas before opening the shutter.

Degassing and first melt

Most spitting is trapped gas or moisture releasing at the first melt. Raise power slowly, hold below evaporation temperature until the pressure recovers, then ramp. Material that has absorbed moisture in storage cannot be fixed at the source.

What we supply

  • All evaporation materials — pellets, granules, pieces and sheets, 2N4 to 7N
  • Al, Ag, Au, Cr, Cu, Ni, Pt, Sn, Ti, V, W and alloys such as AuGeNi and AuSn
  • Custom preforms and arc-cast slugs to drawing

Frequently asked

Pellets or granules — does it change film quality?

Not directly, but it changes melt stability. Pellets give a repeatable fill level; granules fill more densely and are easier to top up mid-run.

Why does my copper pellet spit?

Almost always residual gas or a cold hearth spot. Pre-melt slowly and make sure the beam is not focused on one point.

Do you supply material in a specific liner?

We can supply material pre-loaded in graphite or BN liners to your source geometry, quoted against the drawing.

Related reading: evaporation methods compared · purity grades explained