Reading a certificate of analysis: what ‘99.99%’ actually means

Every supplier will tell you their material is 99.99%. Very few certificates actually let you check that claim, and fewer still let you compare two suppliers on the same basis. This note explains what a certificate of analysis (COA) should contain, where the number can mislead you, and the five questions to ask before you accept a lot.

The problem with “99.99%”

A purity figure is meaningless without a basis. The same copper can honestly be described as 99.99% and 99.95% at the same time:

Stated as 99.99% min, metals basis
Oxygen content 380 ppm (0.038%)
Metals basis impurities among metals sum to < 100 ppm → 99.99%
Total basis 100% − 0.038% oxygen − 0.009% metals = 99.953%

Neither number is a lie. They answer different questions. The trouble starts when a buyer compares a metals-basis certificate against a total-basis certificate and concludes that one supplier is better.

For metals such as copper, aluminium, nickel and titanium, oxygen, nitrogen and hydrogen are routinely excluded from the “metals basis” figure. For oxides and ceramics (ITO, TiO2, Ta2O5) the situation is worse: a target described as 99.99% may be 99.99% cation purity with a stoichiometry that is 2% off, which matters far more to the film than the trace metals do.

What a usable certificate contains

A certificate you can act on has six elements:

  1. Lot number — tied to the actual material in the drum, not to a product family.
  2. Declared purity and its basis — for example “99.99% min, metals basis, oxygen excluded” or “99.995% total”.
  3. An impurity table — element by element, with measured values.
  4. Detection limits — the value below which the instrument cannot see. Without them, a blank cell tells you nothing.
  5. The method used per element — ICP-OES, ICP-MS, GDMS or inert gas fusion.
  6. Laboratory and date — which lab issued the result, and when. “In-house” is acceptable if the lab is named.

If any of the six is missing, the certificate is a marketing document rather than a quality record.

Methods and what they can actually see

ICP-OES ppm to sub-ppm for most metals · routine lot release · cannot see O, N, H, C reliably
ICP-MS ppb range · trace metals for 4N–5N · still blind to gases
GDMS full survey including light elements · the method of choice for 5N+ and for sputtering targets
Inert gas fusion oxygen, nitrogen, hydrogen · essential for vacuum-melt stock and for targets that must not outgas

Two certificates can both say 99.99% while one was produced by ICP-OES with a 1 ppm detection limit and the other by GDMS with a 0.01 ppm limit. The second is not “better material” — it is a closer look at the same material. This is why 5N and 6N claims are only credible when GDMS or ICP-MS is named.

How to compare two certificates

Put them on the same basis before comparing anything:

  1. Normalise the basis. Ask each supplier to state purity on a total basis, including gases. Most will provide it on request.
  2. Check what is reported as “not detected”. A good certificate writes “< 0.5 ppm” or “n.d. (DL 0.1 ppm)”. A poor one writes “0” or leaves the cell empty. Zero is not a measurement.
  3. Look at the elements that matter for your process. For a sputtering target these are usually the ones that form volatile species or segregate: O, C, S, Cl, alkalis. For solder they are oxide formers and anything that raises the melting range.
  4. Check the lot-to-lot spread. One certificate proves one lot. Ask for the last three.

Red flags

  • A purity claim with no impurity table — no table, no basis, no claim.
  • A table where every element reads zero. Real measurements have detection limits.
  • No lot number, or a lot number that is the same across shipments.
  • Method not stated, or a 6N claim analysed by ICP-OES only.
  • Oxide and ceramic targets described only by cation purity, with no stoichiometry or density data.
  • A certificate issued by a trading company that will not name the laboratory.

Five questions to ask before accepting a lot

  1. What is the purity on a total basis, including oxygen, nitrogen and carbon?
  2. Which laboratory issued this certificate, and which method was used for each element?
  3. What are the detection limits for the elements you did not detect?
  4. Can I see the previous three lots for the same grade?
  5. Can I nominate a third-party inspection before shipment?

A supplier who can answer all five without hesitation is telling you something more useful than any single percentage.

What our certificates contain

Every lot we ship carries a certificate stating the lot number, the declared purity and its basis, the impurity table with values and detection limits, the method used per element, and the laboratory that issued the result. Analyses are performed by accredited third-party laboratories; our principal partner is Guobiao (Beijing) Testing & Certification Co., Ltd. Certificates are issued against the lot, not the product family.

If you are qualifying a new grade, ask for a sample with the same lot numbering as production — it is the only way to know that the certificate you are reading describes the material you will receive.

Related reading: how we test and document · purity grades explained · request a quote